400 HDPE Marine Board
| PROPERTY | TEST METHOD |
||
| Melt Index | D1238 | g/10 min | 0.29 |
| Density | D1505 | g/cc | 0.955 |
| Elongation at yield, % | D638 | % | 9 |
| Elongation at break, % | D638 | % | 909 |
| Tensile Strength @ Yield | D638 | psi | 4,050 |
| Tensile Strength @ Break | D638 | psi | 3,400 |
| Flexural Modulus | D790 | psi | 209,200 |
| ESCR (Environmental Stress Crack Resisitance), condition A, F50 | D1693 | h | 35 |
| Vicat softening temperature | D1525 | C(F) | 125(257) |
| HTD (heat deflection temperature) at 66 psi | D648 | C(F) | 77(171) |
| Tensile impact strength | D1822 | ft-lb/in. | 61.3 |
| Shore D hardness | D2240 | 68.5 | |
| Coef. of linear thermal expansion | E831 | in/in/F | 7x10-5 |